1. The stomataThis is a small cavity formed by the gas that cannot be escaped from the metal during solidification. Its inner wall is smooth and contains gas, and it has a high reflectivity to ultrasonic wave.

1. The stomata

This is a small cavity formed by the gas that cannot be escaped from the metal during solidification. Its inner wall is smooth and contains gas, and it has a high reflectivity to ultrasonic wave. However, because it is basically spherical or ellipsoidal, it is also a point defect, which affects its reflected amplitude. After forging or rolling, the pores in ingots are compressed into area defects, which are favorable for ultrasonic detection.

2. Shrinkage cavity and porosity

When the casting or ingot is cooled and solidified, the volume should shrink, and the final solidified part can not be replaced by liquid metal, thus forming a void defect. Large and concentrated voids are called shrinkage holes, and small and dispersed voids are called loose. They are generally located in the last solidified part of the ingot or casting center. The inner wall is rough, and there are many impurities and small pores around them. Due to the law of thermal expansion and cold shrinkage, shrinkage holes are inevitable, but they have different shapes, sizes and positions with different processing methods. When they extend to casting or ingot body, they become defects. If the shrinkage cavity is not removed and brought into the forgings, the ingot will become the residual shrinkage cavity (shrinkage cavity residual, residual shrinkage pipe).

3. The slag

Slag inclusion defect is formed when the slag or refractory material on the furnace body breaks off and enters the liquid metal during the melting process and gets involved in the casting or ingot body during pouring. Slag inclusion usually does not exist in a single, often dense state or dispersed in different depths, it is similar to the volume type of defects but often have a certain degree of linearity.

4. The inclusions

Reaction products (such as oxides, sulphides, etc.) in the melting process - non-metallic inclusion, or some components of the metal components of the additive material is not completely melted and residual metal inclusion, such as high density, high melting point components - tungsten, molybdenum, etc.

5. Segregation

The segregation of castings or ingots mainly refers to the composition segregation caused by uneven distribution of components in the smelting process or the melting process of metals. The mechanical properties of regions with segregation are different from the mechanical properties of the entire metal matrix, and the difference beyond the allowable standard range becomes a defect.

6. Casting cracks

Of casting cracks is mainly due to the metal cooling solidification contraction caused by the stress exceeds the limit of material strength, it is related to the shape of the casting design and casting process, also with some high content of impurities in the metal materials caused by cracking sensitivity about (such as sulfur content high brittleness, high phosphorus content with cold brittleness, etc.). Axial crystal cracks may also occur in ingots. If they cannot be forged together in the subsequent open-billet forging, they will remain in the forgings and become internal cracks in the forgings.

7. Cold insulation

This is a kind of stratification peculiar to the casting defects, mainly related to the casting casting process design, when it is pouring liquid metal, due to interruption of splash, double wave, pouring, or from two different directions (or more) metal flow meet, because the liquid metal semi-solid film on the casting cooling formation on the surface of the body and form a membrane of the area of defects.

8. Skull patch

This is when the steel from ladle to mold casting ingot, because pouring interrupt, pause, first poured into the surface of the liquid metal rapidly cooled in air oxidation film formation, continuing pouring new pouring into the liquid metal to break through its turn into steel ingot and formed a kind of stratification (area) defect, it is not in the subsequent breakdown of ingot forging forging close to eliminate.

anisotropy

When casting or steel ingot is cooled and solidified, the cooling speed from the surface to the center is different, so different crystal structures will be formed, which is manifested as anisotropy of mechanical properties, and also leads to anisotropy of acoustic properties, that is, there are different sound velocities and sound attenuation from the center to the surface. The existence of this anisotropy will have a bad effect on the size and position of casting defects in ultrasonic testing.

主站蜘蛛池模板: 东京热加勒比无码少妇 | 99热在线网站 | 丰满的少妇中文HD高清 | 日韩中文字幕免费视频 | 婷婷综合久久狠狠色成人网 | 国自产在线精品一本无码中文 | 伊人成色综合人夜夜久久 | 国产亚洲人成a在线v网站 | 精品久久国产字幕高潮 | 日本少妇三级HD激情在线观看 | 国产日韩一区二区在线 | 琪琪午夜成人理论福利片美容院 | 蜜臀久久99静品久久久久久 | 无码人妻欧美一区二区三区 | 边勾边做1V1H顾慕琛 | 国产大片B站免费观看推荐 亚洲欧美国产国产一区二区 | 野花社区日本免费图片 | 国产69成人精品视频免费 | 日韩丰满少妇无码内射 | 久久久久波多野结衣高潮 | 日本边添边摸边做边爱的网站 | 日本精品久久久久中文字幕乱中年 | 一级黄色欧美 | 看黄A大片爽爽影院免费无码 | 四虎av无码专区亚洲av | 日本精品一二三 | 精品国产午夜肉伦伦影院 | 亚洲色欲久久久综合网 | 任你躁x7X7X7X7在线观看 | 成人亚洲欧美一区二区三区 | 性感一级毛片 | 国产高清久久久 | 免费视频99 | 无码国产精品一区二区免费模式 | 在线播放国产精品三级 | 91在线在线| 偷窥熟女大屁股对白视频 | 人妻无码久久一区二区三区免费 | 性按摩aaaaaa视频 | 亚洲二三区| chinese老太性视频bbw |